Adhesi antara metode pengujian lapisan dan penerapannya
Makalah ini memperkenalkan metode untuk mengukur daya rekat antara lapisan cat anti korosi karet terklorinasi dan produk serupa. Meskipun metode ini hanya dapat membuat penilaian kualitatif, hal ini sangat penting dalam pertimbangan pemilihan bahan pelapis dan sistem pendukungnya karena konsisten dengan penerapan praktis. Alat dan bahan dijelaskan secara rinci, serta tata cara pengujian daya rekat antara primer dan lapisan tengah, and between the top coat and the middle coat. This approach in the industry standard HG/T 2798 in chlorinated rubber coatings have been mentioned.
1. pengantar
Di industri pelapisan, the evaluation of coating adhesion is one of the key factors to ensure the performance and service life of coatings. Makalah ini memperkenalkan metode untuk mengukur daya rekat antara lapisan cat anti korosi karet terklorinasi dan produk serupa.
Adhesi antara metode pengujian lapisan dan penerapannya
2. Tools and materials
In order to test, the adhesion between the layers you need the following tools and materials:
Artist sculpting knife: for cutting coating sample.
The size of the ruler: used for measuring the coating sample.
Scotch tape: Used in the test step to evaluate the coating adhesion performance.
Filter paper: Used to cover the scotch tape over the coating before testing.
3. Metode
3.1 primer and middle layer adhesion between the paint
3.1.1 sample preparation on one side of a plate with a etch primer, two primer for 48 hours after coating (24 jam). Setelah 7 hari, xenon lamp accelerated aging test was performed for 180 jam. Take out the sample, place it for 24 jam, then apply two intermediate coats (24 hours apart), let it stand horizontally and dry for 7 hari, and prepare three qualified samples.
3.1.2 Steps of adhesion test
Hanging from a hook will test sample for 24 hours in the hot and humid test chamber, suhu 50 + 1 ° C, relative humidity is more than 95%.
Immediately after removing the sample, gently cover the filter paper over the painted surface to absorb excess moisture.
Use art sculpting knife blade, in the middle of the test sample location in parallel to the short side, the direction of the interval of 15 mm cutting two treaties line 40 panjangnya mm, cut through the film to the floor.
In the central part where the cutting lines cross, attach the vertical direction of the cutting lines with scotch tape. One end of the tape needs to be turned back 20mm for tearing and pulling.
Press the tape firmly back and forth with your thumb to ensure that it adheres firmly to the coating, then quickly pull one end of the tape at a right Angle to remove the tape.
Check the lacquer film after tearing. If two or more than two pieces of test samples of the primer paint film with an intermediary between paint film does not occur, or strip width under 3 mm, is judged to be “without exception”.
3.2 surface adhesion between the paint and the middle layer
3.2.1 Sample Preparation Apply a phosphating primer to one side of a steel plate for 4 jam, then apply an intermediate primer for 24 jam, then apply a topcoat for 7 hari, and conduct an accelerated xenon lamp aging test for 180 jam. Take out the sample, setelah 24 jam, and a middle tier paint besmear again paint, make its horizontal and drying, 7 days preparation of three pieces of qualified samples.
3.2.2 Adhesion Test Procedure The operation procedure is the same as that in 3.1.2.
Adhesi antara metode pengujian lapisan dan penerapannya
4.4 Kesimpulan
Through the above method of testing, if two or more test samples in the adhesion test, primer and middle layer paint or top paint and middle layer paint do not peel, or peel width is less than 3mm, it is judged as “no abnormality”.
5. Standar referensi
Method described in this article refer to the industry standard HG/T 2798, chlorinated rubber coatings.
Kesimpulan
Is to ensure that the coating adhesion between the layers of one of the important indexes of stable performance and durability. Although this method can only make a qualitative judgment, it is close to the actual use, and has great significance for coating selection and supporting system design. In the paint industry, penilaian adhesi yang akurat akan membantu memastikan kualitas lapisan dan kinerja, sehingga memastikan penerapan pelapisan jangka panjang.